MaxCell®
Pull-Test Information
Cable on Cable vs. Cable in Fabric Innerduct
Test Condition & Method

Pass Fail Criteria : Having no significant external damage on the cable sheath
Cable on Cable
- Minor abrasion at 250m but significant sheath damage at 500m and 750m
- Large amounts of PE flaking observed over longer distances
- Higher pulling tensions and longer pulls may lead to possible signal failure
Cable in Fabric Innerduct
- Very minor abrasion observed on the sheath
- Fabric Innerduct showed a small 75mm tear right where the cables crossed but the tear did not expose the cable to any significant damage Note: The cable was in a 10m continuous loop. Because of this loop the MaxCell saw the head of the cable pass over a minimum of 75 times during the experiment
- Higher pulling tensions and longer pulls possible without damage to the cable
Control: Cable Observation Before Test
Control: Cable Observation After Test

After 250m Cable on Cable
slight damages

After 500m Cable on Cable
cable jacket clearly damaged

After 750m Cable on Cable
cable jacket heavily damaged

Cable in Fabric Innerduct 750m

Cable Sheath Flakes Collected After “Cable on Cable” 750m Test